Properties
| Trademark | Melt Index(g/10min) | Appearance | Grafting Level | Density(g/cm3) | 
| RP | 1.2 | Colorless or white translucent particles | Medium | 0.86-0.89 | 
| RP157 | 0.4 | Colorless or white translucent particles | High | 0.86-0.88 | 
Effects of GT-RP and GT-RP157 on the properties of toughened PA6
| Properties | Measurement | PA6 | PA6+10%(GT-RP) | PA6+10%(GT-RP157) | 
| Tensile Strength | MPa | 67 | 62 | 58 | 
| Bending strength | MPa | 80 | 68 | 53 | 
| Izod impact strength | KJ/m2 | 6.2 | 30 | 48 | 
Effects of GT-RP on the properties of reinforced and toughened PA6 (with 30% GF)
| Properties | Measurement | PA6+30%GF | PA6+30%GF+3(GT-RP) | PA6+30%GF+5%(GT-RP) | 
| Tensile Strength | MPa | 171 | 167 | 160 | 
| Bending strength | MPa | 200 | 196 | 190 | 
| Izod impact strength | KJ/m2 | 15 | 20 | 24 | 
Note: The above data are typical laboratory results, true and reliable, for reference only, and do not make a formal quality commitment.